What the Number Actually Measures

Heat stability, quoted in degrees Celsius, is the most quoted figure on an organic pigment datasheet and the easiest one to misread. It is not a decomposition temperature. It is the highest processing temperature at which a color survived one specific test without a visible shift in shade. Change the test and the number moves.

Three conditions do most of the moving. Dosage: ratings are commonly established at a low loading of about 0.1% pigment, and pale shades usually show heat drift earlier than deep ones because there is less colorant present to mask a change. Residence time: a five-minute molding cycle is a milder test than twenty minutes in an extruder barrel or on a fiber line. Medium: a value measured in polyethylene does not transfer automatically to nylon or PET, where melt temperatures run higher and the polymer chemistry is more aggressive.

One more reading aid. The measured table behind our organic pigments catalog tops out at 300°C. That ceiling should be read as “passed the standard test”: grades clustered there simply exhausted the scale.

Chemistry Sets the Ceiling

Chemical families ladder upward with molecular weight and lattice rigidity, and the site-measured values make the gradient concrete:

Pigment Chemical family Heat stability (°C) Light fastness
Pigment Yellow 12 Diarylide (disazo) 180 3–4
Pigment Yellow 83 Diarylide (disazo) 200 7
Pigment Red 48:1 Monoazo BONA lake (Ba) 240 5–6
Pigment Violet 23 Dioxazine 250 7–8
Pigment Yellow 93 Disazo condensation 280 8
Pigment Yellow 151 Benzimidazolone 290 8
Pigment Red 122 Quinacridone 300 8
Pigment Red 254 DPP (diketopyrrolopyrrole) 300 8

The pattern is structural. Simple unmodified azo chemistry sits low: PY12 and PY83, both diarylide yellows, measure 180°C and 200°C. Building more chemistry into the molecule lifts the rating: disazo condensation yellows such as PY93 reach 280°C, and the benzimidazolone PY151 reaches 290°C with the best migration fastness on the table. Heterocyclic high performers, quinacridone PR 122 and DPP PR 254 among them, sit at the 300°C ceiling with light fastness 8.

Azo count alone is not destiny. PY12 is a disazo yet rates 180°C, below the 240°C of PR48:1, a monoazo BONA lake. What protects a molecule at temperature is bond strength, molecular size and crystal packing, not the number of azo groups. Salt and grade shift values inside a single color index, too: the PR48 family spans 230–250°C across its Ca, Sr and Ba salts, and unstabilized PB15:0 measures 220°C while the stabilized PB15:1 to PB15:4 grades all reach 300°C. Same color index, very different number. Read the suffix.

The Resin Changes the Answer

A 300°C rating does not clear a pigment for every polymer. PR254 carries a site-measured 300°C, yet the same catalog matrix rates it unsuitable for PA6, PET and PC. PY12 is rated suitable in PE and PP but not in PS or ABS. The heat figure is a thermal limit; the resin matrix records chemical compatibility on top of it, and nylon, with its amine residues, is notoriously hard on azo reds. Conversely, stabilized PB15:1 scores suitable across all twelve resin and fiber columns of the table.

Process shape matters as much as resin identity. Injection molding exposes pigment to a short temperature peak. PET fiber spinning, typically run above 280°C with long residence, is a much harsher thermal history: 47 of the 62 catalog grades rate unsuitable for PET fibers, and 49 of 62 for PA fibers. A rating earned in a five-minute polyolefin test can overstate what survives a thirty-minute engineering-resin cycle.

How Much Margin Is Enough?

Practice varies, but a common working rule is to hold 20–30°C between your process peak and the pigment rating, and more when residence is long, when regrind re-enters the stream, or when the product is a fiber. Deep shades and thicker walls buy a little tolerance; pale tints spend it. When the resin outruns the pigment class, move up the chemistry ladder first: a benzimidazolone or DPP grade often solves what a higher loading of a cheaper yellow cannot. For sustained temperatures beyond 300°C, organic options thin out and inorganic pigments such as iron oxides take over.

FAQ

Is a higher heat stability number always the better choice?

No. A pigment only has to survive your process, not a laboratory worst case. PY13, with a site-measured 200°C, colors polyolefins molded at 180°C without trouble and costs a fraction of a 300°C performance grade. Overbuying heat stability spends margin that shade, fastness or price could use better.

Why do two suppliers quote different numbers for the same pigment index?

Because the index does not fix the product. Salt form (PR48:1 versus PR48:3), stabilization (PB15:0 versus PB15:1), particle size and the test protocol itself (dosage, residence time, resin) all move the measured value. When comparing suppliers, compare test conditions, not just the figure.

How is pigment heat stability actually tested?

The common approach molds or presses the pigmented polymer at stepped temperatures, typically near 0.1% dosage with a residence of a few minutes, then compares each plaque against the reference shade visually or by measured color difference. The rating is the last temperature at which the shift stayed acceptable. It is a pass mark in one protocol, not a physical constant.

About the Numbers Behind Our Catalog

Ningbo Ultra Color Co., Ltd supplies solvent dyes, organic pigments, inorganic pigments, effect pigments and additives to plastics and coatings processors. Every organic pigment batch is tested before release, REACH and RoHS compliance is verified, and retain samples are kept for five years. The heat stability figures quoted here come from that same measured catalog.

Scroll to Top